Miller Dynasty 350 AC/DC TIG (GTAW) & Stick (SMAW) Welder¶
Quick-Reference Operator Card¶
1. Pre-Flight Safety & Station Setup Checklist¶
- [ ] FULL UV ARC-FLASH & SKIN PPE: Put on an ANSI Z87.1 auto-darkening welding helmet with low-amp TIG sensors (Shade 9–12), long-sleeve FR welding jacket, soft kidskin/goatskin TIG gloves, and closed-toe leather boots—zero exposed skin. Close the welding curtains and turn ON the fume extractor.
- [ ] NO CHLORINATED SOLVENTS (PHOSGENE HAZARD): Degrease metal ONLY with 100% Acetone (let evaporate completely). NEVER use chlorinated brake cleaner—TIG UV light converts trace chlorinated vapor into lethal phosgene gas.
- [ ] COOLMATE WATER CHILLER ON: If using a water-cooled TIG torch, turn ON the Coolmate chiller and verify active coolant return flow in the reservoir sight glass before striking an arc.
- [ ] 100% PURE ARGON (15 - 20\text{ CFH}): Verify the cylinder is 100% Pure Argon (never MIG \text{Ar/CO}_2 mix), crack the valve open standing to the side, and set flow to 15 - 20\text{ CFH} (7 - 9.5\text{ L/min}).
- [ ] TUNGSTEN PREP & STICK-OUT: Grind a 2% Lanthanated (Blue) tungsten lengthwise (never crosswise) on the dedicated tungsten grinder—sharp needle point for DC steel/stainless; truncated tip for AC aluminum—and mount with 3 - 6\text{ mm} (1/8 - 1/4\text{ in}) stick-out past the gas lens cup.
2. Standard 5-Step AC/DC TIG Welding Workflow¶
- SELECT PROCESS, POLARITY & AMPERAGE CEILING Select TIG HF Impulse on the Dynasty 350 panel. Choose DCEN for steel/stainless or AC Squarewave for aluminum (70\% - 75\% EN Balance; 100 - 120\text{ Hz} Frequency). Set max amperage (~1\text{ A} per 0.001\text{ in} thickness) and post-flow (\ge 1\text{ s} per 10\text{ A}).
- CLEAN BASE METAL & ATTACH WORK CLAMP Wipe joint with Acetone; for aluminum, scrub immediately before welding with a dedicated stainless-steel wire brush (never used on carbon steel). Clamp ground directly to clean bare metal.
- ESTABLISH PUDDLE & DAB FILLER ROD Announce “Cover!“, hold the tungsten 2 - 3\text{ mm} (3/32 - 1/8\text{ in}) off the joint at a 10^\circ - 15^\circ push angle, press the foot pedal to form a shiny puddle, and dab filler rod (15^\circ angle) into the leading edge—never touch filler rod or puddle to the tungsten.
- TAPER PEDAL & HOLD ARGON POST-FLOW Ease off the foot pedal gradually at the end of the bead to prevent crater cracks, and hold the torch stationary over the crater until Argon post-flow finishes (cooled tungsten must stay bright silver).
- MARK HOT, CLOSE ARGON & POWER DOWN Mark hot metal with soapstone (“HOT”), close the Argon cylinder valve tightly, press Purge until gauges drop to zero, turn OFF the Coolmate chiller and Dynasty 350, and re-grind any dipped tungstens.
3. Baseline Setup Matrix (100\% Argon @ 15 - 20\text{ CFH}, 3/32\text{ in} 2% Lanthanated Tungsten)¶
| Material & Thickness | Polarity / Mode | Max Amperage Ceiling | Filler Rod | AC Settings / Technique Notes |
|---|---|---|---|---|
| Mild Steel — 1.6\text{ mm} (16\text{ ga}) | DCEN (HF Start) | 65 - 80\text{ A} | ER70S-2 (1/16\text{ in}) | Sharp needle point; brisk travel; optional 2\text{ PPS} pulse. |
| Mild Steel — 3.2\text{ mm} (1/8\text{ in}) | DCEN (HF Start) | 115 - 135\text{ A} | ER70S-2 (3/32\text{ in}) | Sharp needle point; tight 2 - 3\text{ mm} arc length. |
| 304 Stainless — 1.6\text{ mm} (16\text{ ga}) | DCEN + Pulse | 55 - 70\text{ A} | ER308L (1/16\text{ in}) | Gas lens cup (20\text{ CFH}); keep hot rod tip inside Argon shield. |
| 6061 Aluminum — 3.2\text{ mm} (1/8\text{ in}) | AC Squarewave | 130 - 150\text{ A} | ER4043 (3/32\text{ in}) | Balance: 72\% EN; Freq: 120\text{ Hz}; form puddle before dabbing. |
(Stick / SMAW Mode: Turn OFF Coolmate chiller, disconnect TIG torch & foot pedal, connect stinger to Positive (+) and ground to Negative (-) [DCEP], and select Stick mode.)
4. Rapid TIG Arc & Contamination Troubleshooting¶
| Issue | Root Cause | Immediate Corrective Action |
|---|---|---|
| Spitting, Wandering Arc / Green Flame | Tungsten dipped in puddle/filler rod, or ground on contaminated steel wheel. | Stop immediately, swap in a clean pre-ground tungsten, and re-grind dipped tip lengthwise on the dedicated tungsten wheel. |
| Crusty Black / Blue Tungsten & Grey Weld | Argon cylinder closed, torn back-cap O-ring, draft blowing shield away, or short post-flow. | Verify 15 - 20\text{ CFH} pure Argon, inspect back-cap O-ring, close bay doors/curtains, and increase post-flow to 8 - 10\text{ s}. |
| Black Peppery Soot on Aluminum Weld | AC Balance set too high (> 80\% EN) with insufficient cathodic cleaning, or unbrushed oxide. | Lower AC Balance to 68\% - 72\% EN, wipe with Acetone, and scrub with dedicated stainless brush. |
| Tungsten Tip Melting Into Huge Ball (AC) | AC Balance set too low (\< 60\% EN, excessive EP heat) or amperage too high for tungsten size. | Raise AC Balance toward 72\% - 75\% EN, or step up to a larger 3/32\text{ in} or 1/8\text{ in} tungsten. |
⚠️ CRITICAL CHILLER, UV & PHOSGENE GAS HAZARD: Never weld above 100\text{ A} with a water-cooled torch unless the Coolmate chiller is ON and circulating, never touch the tungsten while pressing the foot pedal, and never clean metal with chlorinated brake cleaner (creates lethal phosgene gas under TIG UV light). At end of session, close the Argon cylinder valve tightly, press Purge to bleed gauges to zero, switch OFF the chiller and Dynasty 350, and re-grind used tungstens.